Test temperatures C |
0.2% Yield strength N/mm2 |
Tensile strength N/mm2 |
Elongation % |
Reduction of area % |
Aluminum brass |
R.T. |
246 |
455 |
39 |
65 |
100 |
234 |
437 |
37 |
63 |
200 |
223 |
410 |
39 |
60 |
300 |
209 |
333 |
26 |
30 |
400 |
129 |
279 |
22 |
23 |
500 |
71 |
157 |
30 |
30 |
90/10 Copper-Nickel (ann.) |
R.T. |
106 |
312 |
45 |
78 |
200 |
89 |
268 |
35 |
78 |
300 |
85 |
258 |
32 |
61 |
400 |
86 |
237 |
30 |
60 |
550 |
79 |
150 |
41 |
40 |
80/20 Copper-Nickel (ann.) |
R.T. |
121 |
329 |
44 |
81 |
200 |
105 |
284 |
38 |
80 |
300 |
90 |
270 |
35 |
76 |
400 |
92 |
250 |
31 |
56 |
550 |
88 |
160 |
17 |
15 |
70/30 Copper-Nickel (ann.) |
R.T. |
144 |
366 |
41 |
75 |
200 |
126 |
318 |
37 |
73 |
300 |
119 |
287 |
35 |
65 |
400 |
104 |
243 |
19 |
15 |
550 |
93 |
175 |
16 |
15 |
Note: This Technical Data is taken from various Technical Books & is only as
an advise to users. Users are requested to take proper guidance before basing any
technical calculation on the above technical data. Mtlexs.com, or its Promoter,
Directors, employees will in no way be responsible for any losses, damage etc. in
any manner whatsoever.
|
View Technical Specifications for :
[
Copper ]
[
Brass ]
[
Cupro Nickel ]
[
Aluminium ]
[
Zinc ]
[
Lead ]
[ ASTM Standards ]
At Mtlexs.com, we cannot make any specific recommendations about the suitability
of a given alloy, temper, or shape for your project or application. All technical
data is for comparison purposes only and is NOT FOR DESIGN. It has been compiled
from sources we believe to be accurate but cannot guarantee. WE CAN NOT BE HELD
RESPONSIBLE FOR ANY SUCH TECHNICAL FAILURE.